A good reformer tube shutdown checklist is written before the furnace cools, not during the outage. Once scaffolding is up and the critical path is live, nobody has time to decide what should be measured.

The cost of getting this wrong is quiet rather than dramatic. You finish the turnaround with a set of readings that cannot be compared to last time, and the next remaining life assessment has nothing solid to stand on.

What follows is the sequence we would want in place, grouped into the six things that have to happen. It assumes a primary reformer in hydrogen, ammonia, methanol or direct reduction service.

Before the furnace comes down

Three things are far easier to capture hot than cold, and all three are routinely missed.

Take a final pyrometer survey at normal firing, from the same positions used in previous surveys, with emissivity corrected and recorded. This is the last chance to see the furnace as it actually ran.

Photograph every tube showing a hot band, bowing or discolouration, with the tube number legible in the frame. Cold tubes hide what hot tubes show plainly.

Record pressure drop per tube against the furnace average. A tube reading low is flowing more gas than its neighbours and is a candidate for catalyst problems.

The six part reformer tube shutdown checklist

1. Measure diameters at fixed positions

Creep strain shows up as permanent diametral growth, so this is the single most useful number you will collect.

Measure at marked elevations, the same ones every outage, and at two orientations at each elevation so that one sided growth is visible. Record the orientation, not just the value.

The rate of change between outages matters more than the absolute figure. A tube that has been stable for two campaigns is in better condition than a lower reading that moved sharply last year.

2. Run non destructive testing with the results mapped

Eddy current testing finds subsurface creep damage and crack initiation. Radiography confirms findings at welds and at anything another method flagged.

The value is in the mapping. Results must be recorded against tube number and elevation so that the same location can be re-examined next time. An unmapped report cannot be trended.

Our own in-house testing capability is organised the same way, with every indication tied to a position rather than a batch.

The six stages of a reformer tube shutdown checklist shown in sequence
The six stages, in the order they should run.

3. Inspect every weld as its own item

Girth welds, cast to wrought transitions and harp connections behave differently from the parent tube. A surprising share of failures investigated as material problems turn out to sit in or beside a weld.

Give each weld a permanent identifier and its own inspection history. Treating welds as part of the tube hides exactly the data you need.

4. Check catalyst condition and packing

Catalyst condition and tube condition are the same conversation. Reforming is endothermic, so where catalyst activity falls the tube wall gets hotter.

Note settling, bridging, breakage and carbon laydown as you unload, tube by tube. Cross-reference that against the hot band photographs taken before shutdown.

Loading matters as much as unloading. Uneven packing density produces uneven flow and the localised heating that follows from it.

5. Service the burners before anything is closed up

Burner alignment and tip condition decide whether the next campaign runs evenly. Flame impingement causes one sided damage that no tube specification can design around.

Check alignment against the drawings rather than by eye, replace worn tips, and record the flame pattern observed on light up for comparison next time.

6. Decide replacements with the lead time in hand

This is the part a reformer tube shutdown checklist usually gets wrong, because it is the part that has to happen months earlier.

Centrifugally cast tubes are made to order. Casting, machining, welding into assemblies, testing and certification all take time, and the alloy grade affects it.

Deciding scope during the outage means either accepting a schedule extension or running tubes you had intended to replace. Set the trigger criteria for replacement before the previous campaign ends.

Handling aged tubes safely

Tubes that have run for years are not the same material that went in. Carbides have coarsened, secondary phases have formed, and room temperature ductility has fallen.

The practical effect is that aged tubes tolerate far less abuse during handling than new ones. A knock that a new casting would shrug off can crack an aged one.

Support removed tubes along their length rather than at the ends. Avoid dropping or dragging them, and do not use them as convenient working platforms once they are on the ground.

Field welding on aged material needs a qualified procedure that accounts for the condition of the metal, not the procedure used at original construction. This applies to both the older and the higher alloyed grades.

If any tubes are being returned for examination, keep them identified by position and protect the bore. A tube that arrives unlabelled tells us very little that is useful.

A realistic planning timeline

Most of this checklist is work that happens well before the outage window opens.

WhenWhat happens
Previous campaignAgree the criteria that will trigger tube replacement
Well before the outageObtain current lead times and reserve casting capacity
Before shutdownFinal pyrometer survey, hot band photographs, pressure drop per tube
Early in the outageDiameter measurement and non destructive testing, mapped
Mid outageWeld inspection, catalyst assessment, burner service
Before closing upRecord positions, grades and heat numbers of everything installed
After start upBaseline survey for the new campaign

The last row is the one most often skipped. A baseline survey taken just after start up is what makes the next set of readings interpretable.

Where replacement tubes are to a different grade from the originals, the comparison is worth documenting too. Our note on higher creep strength grades covers what changes when the specification moves.

The three mistakes that cost the most

Across the outages we are asked about, the same three errors come up repeatedly, and none of them is technical.

The first is measuring in different places each time. Readings taken from unmarked positions cannot be compared, so years of diligent work produce a dataset nobody can trend.

The second is deciding replacement scope inside the outage window. By then the only options are a schedule extension or running tubes that should have come out.

The third is losing the link between a reading and a tube. Aggregate figures for the furnace are nearly useless, because the campaign is decided by the worst tubes rather than the average.

All three are solved with discipline rather than equipment. Marked positions, criteria agreed in advance, and records kept per tube and per weld.

What to document afterwards

The outage record is the input to every future decision, so it is worth more than the time it takes.

RecordLevel of detailWhy it matters later
Diameter readingsPer tube, per elevation, per orientationThe creep trend
NDT indicationsPer tube and positionRe-examination next outage
Weld historyPer weld identifierSeparates weld from parent metal
Catalyst notesPer tubeExplains hot bands
Burner workPer burnerLinks firing to local damage
Tubes replacedPosition, grade, heat numberMixed age tracking
Trip countPer campaignCycling contribution

Record the heat number and grade of every tube installed, with its position. Furnaces end up holding tubes of several ages and sometimes several grades, and nobody can assess that later without the record.

Design and thickness calculations for heater tubes follow ISO 13704:2022, which is the document to cite if replacement tubes are specified to a different basis than the originals.

Questions we are asked most often

How early should replacement tubes be ordered?

Earlier than most schedules assume. Lead time depends on grade, size, quantity and whether assemblies are welded and tested before despatch. Ask for a current figure rather than relying on the last project.

Is eddy current testing enough on its own?

No single method covers every mechanism. Eddy current is strong on subsurface creep damage but should sit alongside diameter measurement, visual records and radiography at welds.

Can tubes of different grades share a harp?

It happens often after partial replacement, and it is manageable, but it changes flow distribution and complicates later assessment. Where practical, replace a full row rather than scattered tubes.

What should be photographed during the outage?

More than most teams bother with. Hot bands and bowing before shutdown, the bore condition of any tube removed, every weld being inspected, and the catalyst as it comes out.

Include the tube number in the frame and shoot from repeatable positions. Photographs taken this way become comparable evidence rather than a folder nobody opens again.

Who should hold the tube records?

Keep them with the plant rather than with a contractor. Inspection vendors change, and a trend that resets every time the contract is retendered has little value.

Uni Abex supplies centrifugally cast reformer tubes and welded assemblies with full test certification. If you are scoping a turnaround and want lead times before you fix the replacement list, send us the tube schedule.

Leave a Reply

Your email address will not be published. Required fields are marked *